Detection of small nonmetallic inclusion

Does anybody know how to detect small non metalic inclusion ( 0,010 mm to 0,020 mm ) into steel ( X51CrMo3 or X51CrMoV5-1 ).
Steel thickness 0,5 mm
Détection on the surface and in the volume.

Thank you


 
 Reply 
 
Jim Kovarik
Jim Kovarik
06:19 Feb-19-2004
Re: Detection of small nonmetallic inclusion
----------- Start Original Message -----------
: Does anybody know how to detect small non metalic inclusion ( 0,010 mm to 0,020 mm ) into steel ( X51CrMo3 or X51CrMoV5-1 ).
: Steel thickness 0,5 mm
: Détection on the surface and in the volume.
: Thank you
------------ End Original Message ------------

A radiographic linear array system should be able to detect these indications.
Lixi Inc. has some experience with these systems. Their website is www.lixi.com


 
 Reply 
 
Francois Blanchard
Francois Blanchard
06:27 Feb-19-2004
Re: Detection of small nonmetallic inclusion
----------- Start Original Message -----------
: Does anybody know how to detect small non metalic inclusion ( 0,010 mm to 0,020 mm ) into steel ( X51CrMo3 or X51CrMoV5-1 ).
: Steel thickness 0,5 mm
: Détection on the surface and in the volume.
: Thank you
------------ End Original Message ------------

You can also investigate the possibility of a laser ultrasonic system. Expensive but able to detect high frequency ultrasound. (www.tecnar.com) With Ghz ultrasound, I was able to measured thickness foil down to 10um.
regards,
Francois




 
 Reply 
 
John Pursley
R & D
Envision Product Design, USA, Joined Oct 1999, 23

John Pursley

R & D
Envision Product Design,
USA,
Joined Oct 1999
23
00:06 Feb-20-2004
Re: Detection of small nonmetallic inclusion
Envision's high resolution digital X-ray panels and linear arrays along with a micro-focus source will image your inclusions in the 10 to 20 micron range. http://cmosxray.com

----------- Start Original Message -----------
: : Does anybody know how to detect small non metalic inclusion ( 0,010 mm to 0,020 mm ) into steel ( X51CrMo3 or X51CrMoV5-1 ).
: : Steel thickness 0,5 mm
: : Détection on the surface and in the volume.
: : Thank you
: You can also investigate the possibility of a laser ultrasonic system. Expensive but able to detect high frequency ultrasound. (www.tecnar.com) With Ghz ultrasound, I was able to measured thickness foil down to 10um.
: regards,
: Francois
------------ End Original Message ------------




 
 Reply 
 
rizal
rizal
01:03 Feb-24-2004
Re: Detection of small nonmetallic inclusion
please comment and give some tips about my research.. topic:
Investigation of crack defect in roof clay product using ultrasonic
machine
thanks alot..



 
 Reply 
 
Zhong Soo Lim
Zhong Soo Lim
01:40 Apr-15-2004
Re: Detection of small nonmetallic inclusion
----------- Start Original Message -----------
: Does anybody know how to detect small non metalic inclusion ( 0,010 mm to 0,020 mm ) into steel ( X51CrMo3 or X51CrMoV5-1 ).
: Steel thickness 0,5 mm
: Détection on the surface and in the volume.
: Thank you
------------ End Original Message ------------

Magnetic Leakage Flux method can be one of the possible candidates, which is good since it is a noncontact method, and no couplant is needed.
I have done a similar research, which is very easy to apply.
The detectivity of the nonmetallic inclusion can be down to 1x10^(-4) mm^(3), or better than that in some cases.
There can be some limitations.

1. Surface condition
2. Uniformity of the inner material structure

The thickness of 0.5 mm can be a problem.
But you can access from both sides (top and bottom).

If you have any question, then we can discuss further.

Zhong Soo Lim



 
 Reply 
 

Product Spotlight

Conformable wedge transducer

The conformability is obtained with a flexible membrane filled with water between the transducer and
...
the inspected component. The coupling between the membrane and the component requires a small quantity of water or couplant. The conformable wedge combines the acoustic performance of immersion technique with good coupling and low attenuation.
>

High-performance Linear Phased Array Probes

Available to order from stock in a range of 5MHz – 7.5MHz and from 16 to 64 elements. Designed w
...
ith piezo-composite elements, Phoenix phased array probes provide high-resolution imaging to maximise sensitivity; accurate ultrasonic detection and sizing of defects in welds; and effective corrosion mapping. Housed in a rugged stainless steel case for on-site industrial NDT applications.
>

FAAST-PA! OEM Patented phased Array for high speed UT inspection

Multiangle, Multifocus, Multifrequency, Multibeam. Instead of stacking UT electronics and having m
...
any PA probes, FAAST-PA is able to transmit all delay laws within ONE single shot in Real time.
>

Wireless TOFD scanner

Quick, accurate and highly reproducible welds testing. The System operates wirelessly and is compat
...
ible with any type of Windows based Laptop, Desktop or Tablet.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window