Detection of small nonmetallic inclusion

Does anybody know how to detect small non metalic inclusion ( 0,010 mm to 0,020 mm ) into steel ( X51CrMo3 or X51CrMoV5-1 ).
Steel thickness 0,5 mm
Détection on the surface and in the volume.

Thank you


 
 Reply 
 
Jim Kovarik
Jim Kovarik
06:19 Feb-19-2004
Re: Detection of small nonmetallic inclusion
----------- Start Original Message -----------
: Does anybody know how to detect small non metalic inclusion ( 0,010 mm to 0,020 mm ) into steel ( X51CrMo3 or X51CrMoV5-1 ).
: Steel thickness 0,5 mm
: Détection on the surface and in the volume.
: Thank you
------------ End Original Message ------------

A radiographic linear array system should be able to detect these indications.
Lixi Inc. has some experience with these systems. Their website is www.lixi.com


 
 Reply 
 
Francois Blanchard
Francois Blanchard
06:27 Feb-19-2004
Re: Detection of small nonmetallic inclusion
----------- Start Original Message -----------
: Does anybody know how to detect small non metalic inclusion ( 0,010 mm to 0,020 mm ) into steel ( X51CrMo3 or X51CrMoV5-1 ).
: Steel thickness 0,5 mm
: Détection on the surface and in the volume.
: Thank you
------------ End Original Message ------------

You can also investigate the possibility of a laser ultrasonic system. Expensive but able to detect high frequency ultrasound. (www.tecnar.com) With Ghz ultrasound, I was able to measured thickness foil down to 10um.
regards,
Francois




 
 Reply 
 
John Pursley
R & D
Envision Product Design, USA, Joined Oct 1999, 23

John Pursley

R & D
Envision Product Design,
USA,
Joined Oct 1999
23
00:06 Feb-20-2004
Re: Detection of small nonmetallic inclusion
Envision's high resolution digital X-ray panels and linear arrays along with a micro-focus source will image your inclusions in the 10 to 20 micron range. http://cmosxray.com

----------- Start Original Message -----------
: : Does anybody know how to detect small non metalic inclusion ( 0,010 mm to 0,020 mm ) into steel ( X51CrMo3 or X51CrMoV5-1 ).
: : Steel thickness 0,5 mm
: : Détection on the surface and in the volume.
: : Thank you
: You can also investigate the possibility of a laser ultrasonic system. Expensive but able to detect high frequency ultrasound. (www.tecnar.com) With Ghz ultrasound, I was able to measured thickness foil down to 10um.
: regards,
: Francois
------------ End Original Message ------------




 
 Reply 
 
rizal
rizal
01:03 Feb-24-2004
Re: Detection of small nonmetallic inclusion
please comment and give some tips about my research.. topic:
Investigation of crack defect in roof clay product using ultrasonic
machine
thanks alot..



 
 Reply 
 
Zhong Soo Lim
Zhong Soo Lim
01:40 Apr-15-2004
Re: Detection of small nonmetallic inclusion
----------- Start Original Message -----------
: Does anybody know how to detect small non metalic inclusion ( 0,010 mm to 0,020 mm ) into steel ( X51CrMo3 or X51CrMoV5-1 ).
: Steel thickness 0,5 mm
: Détection on the surface and in the volume.
: Thank you
------------ End Original Message ------------

Magnetic Leakage Flux method can be one of the possible candidates, which is good since it is a noncontact method, and no couplant is needed.
I have done a similar research, which is very easy to apply.
The detectivity of the nonmetallic inclusion can be down to 1x10^(-4) mm^(3), or better than that in some cases.
There can be some limitations.

1. Surface condition
2. Uniformity of the inner material structure

The thickness of 0.5 mm can be a problem.
But you can access from both sides (top and bottom).

If you have any question, then we can discuss further.

Zhong Soo Lim



 
 Reply 
 

Product Spotlight

Customized Probes and Transducers

With a strong development department and our own piezocomposite production, we accompany you from th
...
e first product idea to serial production. Our scientists are continuously researching new methods in the field of ultrasonic measurement technology. The progress achieved enables us to offer you optimal solutions.
>

PAUT Probes

Typical Phased Array probes have frequencies between 1MHz and 20MHz and the number of wafers is 10
...
to 128. M2 Electronics offers customers conventionally ultrasound probes and the ability to provide high-precision Phased Array Ultrasound Probes of up to 256 wafers. We can also customize the probe for our customers to meet the specific application requirements of the user.
>

OmniScan™ X3 flaw detector

The OmniScan X3 flaw detector is a complete phased array toolbox. Powerful tools, like total focus
...
ing method (TFM) images and advanced visualization capabilities, enable you to complete your inspection with greater confidence.
>

UCI Hardness Tester NOVOTEST T-U2

UCI hardness tester NOVOTEST T-U2 is is used for non-destructive hardness testing of: metals and
...
alloys by scales of hardness: Rockwell (HRC), Brinell (HB), Vickers (HV); non-ferrous metals, alloys of iron etc., and using five additional scales for calibration; with tensile strength (Rm) scale determines the tensile strength of carbon steel pearlitic products by automatic recalculation from Brinell (HB) hardness scale.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window