17:31 Jul-02-2016
Cracking In Carbon Steel

Hello everyone,

All fabrication and inspection is to AWS D1.1. Fabricating utility poles that are tapered with 12 or 18 flats. 1/4-5/8 shaft and 2 1/2 to 4in. flange is the range of raw material as of now. Finding many cracks in weld. Specifically inspecting today a 7/16 in. shaft welded to 3 in. flange. Mig welding a single groove, 45 degree bevel. Welding inner pass first then coming outside and back gouging and laying multiple passes to obtain CJP. Welding parameters are: Wire- Hobart .052 and Lincoln .052, Wire speed- 330, Volts- 26.5, Gas- 90AR 10Co2. Pre-heat- 300 F of flange and shaft"at least 3in. from direct area being welded." Everyone has gotten involved including engineering and owners. Material certs have been checked as well as WPS's verified as ok for our application. Cannot find solution. Found multiple defects with height reading as 1/4 to 7/16. Welder arc gouged and did find cracks. Then ground to specified height reading and re-welded. No verification that defect was gone with any other NDT method. When I checked with UT same indication and identical characteristics on A-scan as first inspection but now 000"- 5/16. Welder arc-gouged in and indeed found cracks again even though welder claimed that all defects were gone when he began welding for the repair. I'm being questioned as the UT tech of whether or not I'm giving accurate measurements. Is it possible for cracks to propagate height wise through the volume of the weld and why are we having so much cracking in the first place?

 
 Reply 
 
Mark
,
Zambia, Joined Jun 2016, 49

Mark

,
Zambia,
Joined Jun 2016
49
07:54 Jul-03-2016
Re: Cracking In Carbon Steel
In Reply to John Lomax at 17:31 Jul-02-2016 (Opening).

John,
Can you upload any sketch of bevel configuration or WPS?

 
 Reply 
 
Heydar Alakbarov
NDT Inspector,
Inspection Services, Inc., USA, Joined May 2016, 8

Heydar Alakbarov

NDT Inspector,
Inspection Services, Inc.,
USA,
Joined May 2016
8
01:52 Jul-05-2016
Re: Cracking In Carbon Steel
In Reply to John Lomax at 17:31 Jul-02-2016 (Opening).

John,
I recommend to verify metal soundness after air gouging by using MT. Very often visually it looks like crack removed but when you apply MT you see reminded crack which expanded during rewelding.

 
 Reply 
 
John
NDT Inspector,
USA, Joined Jul 2016, 6

John

NDT Inspector,
USA,
Joined Jul 2016
6
13:03 Jul-05-2016
Re: Cracking In Carbon Steel
In Reply to Mark at 07:54 Jul-03-2016 .

zoom image



Hopefully you can see it.
 
 Reply 
 
Paul Holloway
Consultant,
Holloway NDT & Engineering Inc , Canada, Joined Apr 2010, 218

Paul Holloway

Consultant,
Holloway NDT & Engineering Inc ,
Canada,
Joined Apr 2010
218
17:32 Jul-05-2016
Re: Cracking In Carbon Steel
In Reply to John at 13:03 Jul-05-2016 .

Hi John,

Can you sketch exactly where the cracks are showing up? It's too bad you are being questioned as to your accuracy when upon excavation the cracks are visible. I've seen this happen alot and it's very frustrating... we're always the bearer of bad news!

-Paul

 
 Reply 
 
John
NDT Inspector,
USA, Joined Jul 2016, 6

John

NDT Inspector,
USA,
Joined Jul 2016
6
18:04 Jul-05-2016
Re: Cracking In Carbon Steel
In Reply to Paul Holloway at 17:32 Jul-05-2016 .

Hi Paul,

I would say 90% of the time it's between the inner pass and root pass. A lot of times I also find cracking on the knuckles where the weld profile is concave, in the scenario it's almost always center line cracking.


 
 Reply 
 
John
NDT Inspector,
USA, Joined Jul 2016, 6

John

NDT Inspector,
USA,
Joined Jul 2016
6
17:25 Jul-06-2016
Re: Cracking In Carbon Steel
In Reply to Paul Holloway at 17:32 Jul-05-2016 .

Hi Paul,

I would say 90% of the time it's between the inner pass and root pass. A lot of times I also find cracking on the knuckles where the weld profile is concave, in the scenario it's almost always center line cracking.


 
 Reply 
 

Product Spotlight

OmniScan™ X3 flaw detector

The OmniScan X3 flaw detector is a complete phased array toolbox. Powerful tools, like total focus
...
ing method (TFM) images and advanced visualization capabilities, enable you to complete your inspection with greater confidence.
>

HARDNESS TESTER TKM-459CE combi

TKM-459CE combi applies 2 methods of hardness control: UCI and Leeb. It provides high-accuracy tes
...
ting of metals and alloys as well as items of different sizes and configurations, their hardened layers and galvanic coatings. Device represents results in HB, HRC, HV and others. Shock-, dust- and water-proof housing with intuitive software make this gauge easy to use in all working conditions.
>

Wireless TOFD scanner

Quick, accurate and highly reproducible welds testing. The System operates wirelessly and is compat
...
ible with any type of Windows based Laptop, Desktop or Tablet.
>

ISAFE3 Intrinsically Safe Sensor System

ISAFE3 intrinsically safe sensor system of Vallen Systeme is especially targeted at the petrochemica
...
l - as well as oil and gas transportation industry. The sensor system is designed for permanent monitoring or periodic inspection tasks. Sensors are available for different AE-frequency ranges optimized for corrosion and fatigue crack detection and other applications. The ISAFE 3 sensor system consists of an AE-sensor (model ISAS3) certified according to ATEX/IEC for installation in zone 0, gas group IIC, IP68, 20 to +60 °C, and a signal isolator (model SISO3) certified for installation in zone 2. An ISAS3 sensor can be mounted in atmosphere or submerged, e.g. in water or crude oil. It is supported by mounting tools for temporary (magnets) or permanent (welded) installation. ISAFE3 supports automatic sensor coupling test and can be used with any AE signal processor supporting 28V supply at 90 mA peak, e.g. Vallen Systeme ASIP-2/A.
>