17:31 Jul-02-2016
Cracking In Carbon Steel

Hello everyone,

All fabrication and inspection is to AWS D1.1. Fabricating utility poles that are tapered with 12 or 18 flats. 1/4-5/8 shaft and 2 1/2 to 4in. flange is the range of raw material as of now. Finding many cracks in weld. Specifically inspecting today a 7/16 in. shaft welded to 3 in. flange. Mig welding a single groove, 45 degree bevel. Welding inner pass first then coming outside and back gouging and laying multiple passes to obtain CJP. Welding parameters are: Wire- Hobart .052 and Lincoln .052, Wire speed- 330, Volts- 26.5, Gas- 90AR 10Co2. Pre-heat- 300 F of flange and shaft"at least 3in. from direct area being welded." Everyone has gotten involved including engineering and owners. Material certs have been checked as well as WPS's verified as ok for our application. Cannot find solution. Found multiple defects with height reading as 1/4 to 7/16. Welder arc gouged and did find cracks. Then ground to specified height reading and re-welded. No verification that defect was gone with any other NDT method. When I checked with UT same indication and identical characteristics on A-scan as first inspection but now 000"- 5/16. Welder arc-gouged in and indeed found cracks again even though welder claimed that all defects were gone when he began welding for the repair. I'm being questioned as the UT tech of whether or not I'm giving accurate measurements. Is it possible for cracks to propagate height wise through the volume of the weld and why are we having so much cracking in the first place?

 
 Reply 
 
Mark
,
Zambia, Joined Jun 2016, 49

Mark

,
Zambia,
Joined Jun 2016
49
07:54 Jul-03-2016
Re: Cracking In Carbon Steel
In Reply to John Lomax at 17:31 Jul-02-2016 (Opening).

John,
Can you upload any sketch of bevel configuration or WPS?

 
 Reply 
 
Heydar Alakbarov
NDT Inspector,
Inspection Services, Inc., USA, Joined May 2016, 8

Heydar Alakbarov

NDT Inspector,
Inspection Services, Inc.,
USA,
Joined May 2016
8
01:52 Jul-05-2016
Re: Cracking In Carbon Steel
In Reply to John Lomax at 17:31 Jul-02-2016 (Opening).

John,
I recommend to verify metal soundness after air gouging by using MT. Very often visually it looks like crack removed but when you apply MT you see reminded crack which expanded during rewelding.

 
 Reply 
 
John
NDT Inspector,
USA, Joined Jul 2016, 6

John

NDT Inspector,
USA,
Joined Jul 2016
6
13:03 Jul-05-2016
Re: Cracking In Carbon Steel
In Reply to Mark at 07:54 Jul-03-2016 .

zoom image



Hopefully you can see it.
 
 Reply 
 
Paul Holloway
Consultant,
Holloway NDT & Engineering Inc , Canada, Joined Apr 2010, 218

Paul Holloway

Consultant,
Holloway NDT & Engineering Inc ,
Canada,
Joined Apr 2010
218
17:32 Jul-05-2016
Re: Cracking In Carbon Steel
In Reply to John at 13:03 Jul-05-2016 .

Hi John,

Can you sketch exactly where the cracks are showing up? It's too bad you are being questioned as to your accuracy when upon excavation the cracks are visible. I've seen this happen alot and it's very frustrating... we're always the bearer of bad news!

-Paul

 
 Reply 
 
John
NDT Inspector,
USA, Joined Jul 2016, 6

John

NDT Inspector,
USA,
Joined Jul 2016
6
18:04 Jul-05-2016
Re: Cracking In Carbon Steel
In Reply to Paul Holloway at 17:32 Jul-05-2016 .

Hi Paul,

I would say 90% of the time it's between the inner pass and root pass. A lot of times I also find cracking on the knuckles where the weld profile is concave, in the scenario it's almost always center line cracking.


 
 Reply 
 
John
NDT Inspector,
USA, Joined Jul 2016, 6

John

NDT Inspector,
USA,
Joined Jul 2016
6
17:25 Jul-06-2016
Re: Cracking In Carbon Steel
In Reply to Paul Holloway at 17:32 Jul-05-2016 .

Hi Paul,

I would say 90% of the time it's between the inner pass and root pass. A lot of times I also find cracking on the knuckles where the weld profile is concave, in the scenario it's almost always center line cracking.


 
 Reply 
 

Product Spotlight

NOVO Armor 15 & NOVO Armor 22

The Armor Kit Contains the NOVO Armor, which provides additional mechanical protection to the NOVO 1
...
5WN & NOVO 22WN Detectors, the Armor Stand and a traveling soft cover. - Newest shock absorbent technology case - Water resistant design - Supports wired & wireless communication - Multiple positioning options - Tripod connection using the Built-in 1/4” threads - Simple Detector battery replacement
>

EKOSCAN Phased Array

In order to always fit your needs, EKOSCAN can manufacture any type of UT transducer, either convent
...
ional or Phased Array. As an ISO 9001: 2015 certified company, EKOSCAN is extremely careful as far a material selection and manufacturing processes are concerned. Our probes guarantee our customers the benefits of latest innovations regarding piezo-composite, backing, impedance adaptation layer, etc. Specific probes for hostile environment: high temperature, high pressure, corrosive environment,etc. Specific probes designed to fit your specific application: optimization of every parameter to guarantee you the best detection.
>

NEW Wheel Type Phased Array Probe

DOPPLER NEW Wheel Type Phased Array Probe, more stable, new tyre makes lesser acoustic attenuation
...
, much lighter makes easier to handle, more slim size, magnetic and mechanical encoder optional etc...more
>

Compact NDT inspection-heads for measurements with active thermography

The compact inspection head is suitable for thermographic ndt tasks. The uncooled infrared camera
...
is specially developed for NDI-tasks and offers a thermal sensitivity until now known only from thermal imagers with cooled detector. All required components and functions are integrated into the inspection-head. You will only need an ethernet cable to connect the sensor with the evaluation system.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window