bonding piezoelectric ceramics

I have some piezoelectric ceramic discs which i want to attach to a plate to do some work with lamb waves. However, the piezos have electrodes on each side of the disc and do not wrap round. Does anyone have any ideas on how to bond them properly to the plate.
Thanks
Cheryl


 
 Reply 
 
Joerg Schulze-Clewing
Joerg Schulze-Clewing
01:40 Mar-23-2004
Re: bonding piezoelectric ceramics
Cheryl, can you bond wire to the electrode, for example using
conductive epoxy and then glue them? As long as you don't
use high power levels this could work.

Regards, Joerg.

----------- Start Original Message -----------
: I have some piezoelectric ceramic discs which i want to attach to a plate to do some work with lamb waves. However, the piezos have electrodes on each side of the disc and do not wrap round. Does anyone have any ideas on how to bond them properly to the plate.
: Thanks
: Cheryl
------------ End Original Message ------------




 
 Reply 
 
Cheryl Forrester
Cheryl Forrester
01:46 Mar-23-2004
Re: bonding piezoelectric ceramics
would it be possible to use a conductive glue then use the plate as the 2nd electrode. I need to put three discs on the same plate so could this work?
Thanks
Cheryl

----------- Start Original Message -----------
: Cheryl, can you bond wire to the electrode, for example using
: conductive epoxy and then glue them? As long as you don't
: use high power levels this could work.
: Regards, Joerg.
: : I have some piezoelectric ceramic discs which i want to attach to a plate to do some work with lamb waves. However, the piezos have electrodes on each side of the disc and do not wrap round. Does anyone have any ideas on how to bond them properly to the plate.
: : Thanks
: : Cheryl
------------ End Original Message ------------




 
 Reply 
 
Robert Paynter
Robert Paynter
09:18 Mar-23-2004
Re: bonding piezoelectric ceramics
----------- Start Original Message -----------
... piezos have electrodes on each side of the disc and do not wrap round. Does anyone ...
------------ End Original Message ------------

I think you may need to get different piezo discs. Could you not get them attached to a foil on one
side, with one of the electrodes attached to the
foil? Here's a sounder like that.

0.15 GPB - that's pretty good price - I suspect
you will be able to get higher spec ones elsewhere
I suspect the foil/plate it's already attached to
maybe too thick (but maybe not)

Good Luck

Robert



 
 Reply 
 
Joerg Schulze-Clewing
Joerg Schulze-Clewing
00:15 Mar-23-2004
Re: bonding piezoelectric ceramics
Cheryl, you could probably do that. I don't know
your application. My work is medical (so we use PZT-5)
and glueing on a steel plate doesn't really work there
because you'll get a lot of ringdown in the near field,
and poor target resolution. But if you have a CW case
then I guess it won't matter. Just make sure stuff doesn't
corrode much.

Another concern is ground. Mostly I need to have the
front electrode grounded for noise immunity. In your
case that may not be possible because you want to glue
multiple transducers on the same steel plate. So then
the steel would be the common ground.

One other suggestion: You could also used copper clad
circuit board material if you need the back electrodes
of the three transducers separate. It's just not a very
good "backing material". But if you make the copper clad
larger than the transducers then you'd have a place to
solder your cable to.

Regards, Joerg.

----------- Start Original Message -----------
: would it be possible to use a conductive glue then use the plate as the 2nd electrode. I need to put three discs on the same plate so could this work?
: Thanks
: Cheryl
: : Cheryl, can you bond wire to the electrode, for example using
: : conductive epoxy and then glue them? As long as you don't
: : use high power levels this could work.
: : Regards, Joerg.
: : : I have some piezoelectric ceramic discs which i want to attach to a plate to do some work with lamb waves. However, the piezos have electrodes on each side of the disc and do not wrap round. Does anyone have any ideas on how to bond them properly to the plate.
: : : Thanks
: : : Cheryl
------------ End Original Message ------------




 
 Reply 
 
Klaus Brebøl
Klaus Brebøl
08:02 Mar-24-2004
Re: bonding piezoelectric ceramics
----------- Start Original Message -----------
: ... piezos have electrodes on each side of the disc and do not wrap round. Does anyone ...
: I think you may need to get different piezo discs. Could you not get them attached to a foil on one
: side, with one of the electrodes attached to the
: foil? Here's a sounder like that.
: 0.15 GPB - that's pretty good price - I suspect
: you will be able to get higher spec ones elsewhere
: I suspect the foil/plate it's already attached to
: maybe too thick (but maybe not)
: Good Luck
: Robert
------------ End Original Message ------------
If you are working at room temperature you can use the piezos you have. Changing temperatures can give problems, depending on geometry, due to difference in thermal expansion and a thin glue layer. Roughen the surface of the metal with emerycloth. Glue the parts together with a low viscosity glue (like water), epoxy or cyanoacrylate. Keep the parts under light pressure while curing. That will make electrical contact through the glue. Check the capacitance between top electrode on piezo and metal. If it is the same as for the piezo, contact is OK, if not then you have made a series connection of a piezo and a 'glue' capacitor. Cyano glue has the advantage that it dissolves in acetone, so you can try again.

Good luck

Klaus Brebøl





 
 Reply 
 
Cesar Quintero
Cesar Quintero
08:11 Feb-15-2005
bonding piezoelectric ceramics
This page is very important for my job. please, I need now how I can request a epoxic resin for a piezoelectric ceramic that stick to the aluminium piece for treatment medical in phisiotherapy?, thaks.


 
 Reply 
 

Product Spotlight

IRIS 9000Plus - Introducing the next generation of heat exchanger inspection.

Representing the seventh generation of the IRIS system, the IRIS 9000 Plus has nearly 200 years of c
...
ombined field inspection experience incorporated in its design. This experience combined with a strong commitment to quality and a history of innovation has made Iris Inspection Services® the undisputed leader in IRIS technology.
>

Scatter Correction for Industrial Cone-Beam Computed Tomography (CBCT)

Download our white paper on Scatter Correction for Industrial Cone-Beam Computed Tomography (CBCT)
...
Using 3D VSHARP, a fast GPU-Based Linear Boltzmann Transport Equation Solver here: http://bit.ly/2Y0t78P
>

Wireless TOFD scanner

Quick, accurate and highly reproducible welds testing. The System operates wirelessly and is compat
...
ible with any type of Windows based Laptop, Desktop or Tablet.
>

High-performance Linear Phased Array Probes

Available to order from stock in a range of 5MHz – 7.5MHz and from 16 to 64 elements. Designed w
...
ith piezo-composite elements, Phoenix phased array probes provide high-resolution imaging to maximise sensitivity; accurate ultrasonic detection and sizing of defects in welds; and effective corrosion mapping. Housed in a rugged stainless steel case for on-site industrial NDT applications.
>