Hai Experts,
Is PAUT possible for the following joints..

1)Volumetric examination and bond line integrity check in cladded area.

cladded Pipe OD/Material=24"/ API 5L X65
Cladding material & thickness=Inconel 625 & 4.3 mm thickness.
Is there any special Probe like DMA or DLA required?

2)Volumetric Examination in butt joint/similar welds

Butt joint= similar welds ,single 'V' between cladded pipe and cladded hanger flange.

 
 Reply 
 
Aniss Ziani
, Advanced NDT inspector
ISQ, Algeria, Joined Nov 2014, 32

Aniss Ziani

, Advanced NDT inspector
ISQ,
Algeria,
Joined Nov 2014
32
15:12 Mar-11-2017
Re: PAUT in Inconel cladding
In Reply to sreejith at 02:21 Mar-11-2017 (Opening).

Hi Sreejith,
Have a look on this interesting article from Carlo Romito and Frederic Jacques :
https://www.linkedin.com/pulse/method-automatic-ultrasonic-testing-aut-corrosion-resistant-romito-1
Regards,
Aniss Ziani

 
 Reply 
 
Anmol Birring
Consultant,
Birring NDE Center, Inc., USA, Joined Aug 2011, 832

Anmol Birring

Consultant,
Birring NDE Center, Inc.,
USA,
Joined Aug 2011
832
22:24 Mar-11-2017
Re: PAUT in Inconel cladding
In Reply to sreejith at 02:21 Mar-11-2017 (Opening).

what is the weld material ?

 
 Reply 
 
sreejith
India, Joined Jan 2015, 5

sreejith

India,
Joined Jan 2015
5
02:24 Mar-13-2017
Re: PAUT in Inconel cladding
In Reply to Anmol Birring at 22:24 Mar-11-2017 .

SMAW,E7018

 
 Reply 
 
Anmol Birring
Consultant,
Birring NDE Center, Inc., USA, Joined Aug 2011, 832

Anmol Birring

Consultant,
Birring NDE Center, Inc.,
USA,
Joined Aug 2011
832
05:48 Mar-13-2017
Re: PAUT in Inconel cladding
In Reply to sreejith at 02:24 Mar-13-2017 .

So it is carbon steel weld with A625 clad overlay ?

 
 Reply 
 
sreejith
India, Joined Jan 2015, 5

sreejith

India,
Joined Jan 2015
5
07:26 Mar-14-2017
Re: PAUT in Inconel cladding
In Reply to Anmol Birring at 05:48 Mar-13-2017 .

yes

 
 Reply 
 
Anmol Birring
Consultant,
Birring NDE Center, Inc., USA, Joined Aug 2011, 832

Anmol Birring

Consultant,
Birring NDE Center, Inc.,
USA,
Joined Aug 2011
832
04:19 Mar-16-2017
Re: PAUT in Inconel cladding
In Reply to sreejith at 07:26 Mar-14-2017 .

If the weld is CS, you can use PAUT - shear wave but limited to the 1/2 vee mode. So that will mean removal of weld cap to get full weld coverage. And since it is CS you can add TOFD

 
 Reply 
 

Product Spotlight

High-performance Linear Phased Array Probes

Available to order from stock in a range of 5MHz – 7.5MHz and from 16 to 64 elements. Designed w
...
ith piezo-composite elements, Phoenix phased array probes provide high-resolution imaging to maximise sensitivity; accurate ultrasonic detection and sizing of defects in welds; and effective corrosion mapping. Housed in a rugged stainless steel case for on-site industrial NDT applications.
>

GUL Subsea Solutions - Screeening & Monitoring

To inspect new and existing subsea lines, you need proven technology and experience. GUL offers it's
...
technology to solve this challenge: GUL Subsea and gMAT Transducer Rings.
>

NEW - TD Focus-ScanRX

The NEW Next Generation Advanced UT platform, TD Focus ScanRX - Also available as a card stack solut
...
ion. Key Improvements 1. Data acquisition is significantly faster than current design 2. Better aesthetic – closely aligns with HandyScan RX 3. Improved IP rating (Target IP66) 4. Ruggedized housing 5. Connectors are protected from impact and ingress 6. Integrated stand and separate retractable handle easy to keep clean) 7. Touchscreen with ruggedized display glass 8. 3-Axis encoder input
>

Wireless TOFD scanner

Quick, accurate and highly reproducible welds testing. The System operates wirelessly and is compat
...
ible with any type of Windows based Laptop, Desktop or Tablet.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window