New edition of CSA W59 (2018) - changes to UT of welds

CSA has released the 2018 edition of W59 Welded Steel Construction, which includes major changes to the ultrasonic testing of structural welds. These include:

- selection of a variety of probe sizes and frequencies
- use of DAC/TCG for sensitivity calibration
- allowance for manual phased array

These are part of Annex X, which may be used instead of the classic fixed attenuation (FA) techniques in Clause 8.2.

 
 Reply 
 
THEO MICOTTIS
Italy, Joined May 2013, 82

THEO MICOTTIS

Italy,
Joined May 2013
82
09:55 Jun-26-2018
Re: New edition of CSA W59 (2018) - changes to UT of welds
In Reply to Paul Holloway at 09:37 Jun-26-2018 (Opening).

Hi Paul,currently I don't have 2018 edition so I couldn't read it. Annex X can be used only be used with permission of engineer like previous annexes in older editions? Regards
Theo

 
 Reply 
 
Paul Holloway
Consultant,
Holloway NDT & Engineering Inc , Canada, Joined Apr 2010, 233

Paul Holloway

Consultant,
Holloway NDT & Engineering Inc ,
Canada,
Joined Apr 2010
233
13:04 Jun-26-2018
Re: New edition of CSA W59 (2018) - changes to UT of welds
In Reply to THEO MICOTTIS at 09:55 Jun-26-2018 .

Hi Theo, great question.

I will make reference to the fixed attenuation technique in Clause 8.2 as the “FA technique”, and the new technique in Annex X as the “TCG technique”. That will save me from restating it multiple times below.

The TCG technique applies to manual conventional UT and manual PAUT and does not require engineering approval, but may be used "where agreed upon by the contractor and the welding inspection organization." Keep in mind this applies to *manual* UT/PAUT only, where probe oscillation and rastering is possible in order to maximize indication height. Encoded PAUT and other alternate techniques such as TOFD still require engineering approval as per Clause 8.2.12. Of course, in the long term we would all like encoded PAUT to be commonplace, but going all the way from an approach developed in 1969 to full-on encoded PAUT was inconceivably complex and would be impossible to achieve consensus on. As a result, we elected to develop a TCG approach and adopt manual PAUT as a first step.

I should point out that Annex X contains acceptance criteria modified to work with the TCG technique and provide quality levels consistent with the FA technique. So if you use Annex X, you use the new acceptance criteria. If you use the FA technique, then you keep doing things the way you were doing it before and use Tables 11.3 and 12.5. The acceptance levels in Annex X differ by a few dB from those in 11.3 and 12.5, which is due to the differences between actual attenuation and the linear estimation of 2 dB/inch. There is a white paper available on this published in the AWS Welding Journal in March 2018.

1
 
 Reply 
 
M G
,
Canada, Joined Nov 2017, 6

M G

,
Canada,
Joined Nov 2017
6
11:35 Jun-28-2018
Re: New edition of CSA W59 (2018) - changes to UT of welds
In Reply to Paul Holloway at 09:37 Jun-26-2018 (Opening).

Hi, Paul

I haven't got the CSA W59 (2018), have few questions about the old version.
For the welds less than 8 mm, just tell the client we couldn't do it because there is not acceptance criteraia?

 
 Reply 
 
Paul Holloway
Consultant,
Holloway NDT & Engineering Inc , Canada, Joined Apr 2010, 233

Paul Holloway

Consultant,
Holloway NDT & Engineering Inc ,
Canada,
Joined Apr 2010
233
19:02 Jun-28-2018
Re: New edition of CSA W59 (2018) - changes to UT of welds
In Reply to M G at 11:35 Jun-28-2018 .

You are correct.

 
 Reply 
 
M G
,
Canada, Joined Nov 2017, 6

M G

,
Canada,
Joined Nov 2017
6
07:41 Jul-01-2018
Re: New edition of CSA W59 (2018) - changes to UT of welds
In Reply to Paul Holloway at 19:02 Jun-28-2018 .

Thanks

Sometimes we are requested to do SW on pipe welds with W59 because those pipe will be hit into ground as the base of top structure.
How can we scan the circ welds on 16"x 1/2" pipe(Might be smaller size) with the big monster probe as required by W59 , curve the wedge?

 
 Reply 
 
Paul Holloway
Consultant,
Holloway NDT & Engineering Inc , Canada, Joined Apr 2010, 233

Paul Holloway

Consultant,
Holloway NDT & Engineering Inc ,
Canada,
Joined Apr 2010
233
21:33 Jul-01-2018
Re: New edition of CSA W59 (2018) - changes to UT of welds
In Reply to M G at 07:41 Jul-01-2018 .

I would hazard against using curved wedges with the FA technique as it will complicate the calibration. Besides, on a diameter as large as 16 inches I doubt it would amount to much difference.

Keep in mind that with the alternative in Annex X, you can now use much more appropriate search unit sizes and frequencies. Your application would be a great way to show your client the benefit of the recent changes.

 
 Reply 
 
Stan
NDT Inspector,
Canada, Joined Jan 2009, 31

Stan

NDT Inspector,
Canada,
Joined Jan 2009
31
15:52 Jul-02-2018
Re: New edition of CSA W59 (2018) - changes to UT of welds
In Reply to Paul Holloway at 21:33 Jul-01-2018 .

Paul, thanks for this, it’s been a long time coming.
Do you know if the Code has been released yet, and when it comes into effect.
Regards
Stan

 
 Reply 
 
Paul Holloway
Consultant,
Holloway NDT & Engineering Inc , Canada, Joined Apr 2010, 233

Paul Holloway

Consultant,
Holloway NDT & Engineering Inc ,
Canada,
Joined Apr 2010
233
22:28 Jul-03-2018
Re: New edition of CSA W59 (2018) - changes to UT of welds
In Reply to Stan at 15:52 Jul-02-2018 .

Hi Stan:

It was released early June and is in effect now.

It is available on the CSA webstore, and will eventually make it's way into Techstreet and other sources.

Paul

 
 Reply 
 

Product Spotlight

ISONIC 3510

Very Powerful Superior Performance Extremely Portable Smart Phased Array Ultrasonic Flaw Detector an
...
d Recorder with 2 Conventional UT and TOFD Channels uniquely combines PA, single- and multi-channel conventional UT, and TOFD modalities providing 100% raw data recording and imaging. Suitable for all kinds of every-day ultrasonic inspections
>

Customized Probes and Transducers

With a strong development department and our own piezocomposite production, we accompany you from th
...
e first product idea to serial production. Our scientists are continuously researching new methods in the field of ultrasonic measurement technology. The progress achieved enables us to offer you optimal solutions.
>

ISAFE3 Intrinsically Safe Sensor System

ISAFE3 intrinsically safe sensor system of Vallen Systeme is especially targeted at the petrochemica
...
l - as well as oil and gas transportation industry. The sensor system is designed for permanent monitoring or periodic inspection tasks. Sensors are available for different AE-frequency ranges optimized for corrosion and fatigue crack detection and other applications. The ISAFE 3 sensor system consists of an AE-sensor (model ISAS3) certified according to ATEX/IEC for installation in zone 0, gas group IIC, IP68, 20 to +60 °C, and a signal isolator (model SISO3) certified for installation in zone 2. An ISAS3 sensor can be mounted in atmosphere or submerged, e.g. in water or crude oil. It is supported by mounting tools for temporary (magnets) or permanent (welded) installation. ISAFE3 supports automatic sensor coupling test and can be used with any AE signal processor supporting 28V supply at 90 mA peak, e.g. Vallen Systeme ASIP-2/A.
>

Ultrasonic Testing Immersion Tanks with Unmatched Scanning Features

TecScan’s non-destructive testing Ultrasonic Immersion Tanks & scanners are designed for high pe
...
rformance and demanding NDT testing applications. Our Scan3D™ line of High Precision Immersion Tanks are specifically designed for automated ultrasonic testing of complex composites parts used in aerospace and industrial applications.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window