05:30 Feb-01-2000
NDT of Polyurethane Foam

I work for Delphi Interior Systems near Dayton, Ohio. We make
Instrument panels (dashboards) for automobiles using an injection
molding process. This process involves injecting a polyurethane
foam between layers of vinyl and a hard plastic shape retainer.
When the parts are made, especially in the prototype stage, there
are often voids in the foam that may not be detected by the eye
or touch. I am looking for a way to detect the voids non-
destrictively before shipping the parts to the customer. Ideally,
I'd like to find a way to scan the parts and be able to create a
mapping of where the voids occur, and how large they are.
Typically, the voids that cause problems are anywhere from 7-10mm
to a large hole that runs along the length of the part. Please
let me know any ideas you may have, or if your company provides
services and equipment to perform these tests.
Thank you,
Laurie Shopes
Delphi Interior Systems



 
 Reply 
 
Trevor Easton
Engineering
Dofasco Inc, Canada, Joined Nov 1998, 13

Trevor Easton

Engineering
Dofasco Inc,
Canada,
Joined Nov 1998
13
05:58 Feb-01-2000
Re: NDT of Polyurethane Foam
If you can scan the parts immediately after forming you may be able to detect the voids using a thermographic camera. The heating of the foam during expansion may reveal voids as cooler areas on the surface.


: I work for Delphi Interior Systems near Dayton, Ohio. We make
: Instrument panels (dashboards) for automobiles using an injection
: molding process. This process involves injecting a polyurethane
: foam between layers of vinyl and a hard plastic shape retainer.
: When the parts are made, especially in the prototype stage, there
: are often voids in the foam that may not be detected by the eye
: or touch. I am looking for a way to detect the voids non-
: destrictively before shipping the parts to the customer. Ideally,
: I'd like to find a way to scan the parts and be able to create a
: mapping of where the voids occur, and how large they are.
: Typically, the voids that cause problems are anywhere from 7-10mm
: to a large hole that runs along the length of the part. Please
: let me know any ideas you may have, or if your company provides
: services and equipment to perform these tests.
: Thank you,
: Laurie Shopes
: Delphi Interior Systems




 
 Reply 
 
Rich Martin
Rich Martin
06:17 Feb-01-2000
Re: NDT of Polyurethane Foam
You may want to consider low frequency air coupled
ultrasonics as an option. The low frequency allows
through transmission inspection of highly attenuating
materials such as honeycomb structures or as in your
case, foam. I'm not sure if such a system can meet
your flaw size requirements, but it is a relatively
inexpensive method.


: I work for Delphi Interior Systems near Dayton, Ohio. We make
: Instrument panels (dashboards) for automobiles using an injection
: molding process. This process involves injecting a polyurethane
: foam between layers of vinyl and a hard plastic shape retainer.
: When the parts are made, especially in the prototype stage, there
: are often voids in the foam that may not be detected by the eye
: or touch. I am looking for a way to detect the voids non-
: destrictively before shipping the parts to the customer. Ideally,
: I'd like to find a way to scan the parts and be able to create a
: mapping of where the voids occur, and how large they are.
: Typically, the voids that cause problems are anywhere from 7-10mm
: to a large hole that runs along the length of the part. Please
: let me know any ideas you may have, or if your company provides
: services and equipment to perform these tests.
: Thank you,
: Laurie Shopes
: Delphi Interior Systems




 
 Reply 
 
Norm Woodward
Norm Woodward
05:11 Feb-03-2000
Re: NDT of Polyurethane Foam
: You may want to consider low frequency air coupled
: ultrasonics as an option. The low frequency allows
: through transmission inspection of highly attenuating
: materials such as honeycomb structures or as in your
: case, foam. I'm not sure if such a system can meet
: your flaw size requirements, but it is a relatively
: inexpensive method.

:
: : I work for Delphi Interior Systems near Dayton, Ohio. We make
: : Instrument panels (dashboards) for automobiles using an injection
: : molding process. This process involves injecting a polyurethane
: : foam between layers of vinyl and a hard plastic shape retainer.
: : When the parts are made, especially in the prototype stage, there
: : are often voids in the foam that may not be detected by the eye
: : or touch. I am looking for a way to detect the voids non-
: : destrictively before shipping the parts to the customer. Ideally,
: : I'd like to find a way to scan the parts and be able to create a
: : mapping of where the voids occur, and how large they are.
: : Typically, the voids that cause problems are anywhere from 7-10mm
: : to a large hole that runs along the length of the part. Please
: : let me know any ideas you may have, or if your company provides
: : services and equipment to perform these tests.
: : Thank you,
: : Laurie Shopes
: : Delphi Interior Systems

If you decide to look into low frequency, air-coupled devices, one source that I am aware of is NDT Systems of Huntington Beach CA. As I recall, their Curlin Air system has originally developed for the inspection of foam structures.

They can be reached at 714-893-2438, or thru their web site at www.ndtsystems.com.

Norm


 
 Reply 
 
J. Mark Davis
Teacher, And Consultant
University of Ultrasonics, Birmingham, Alabama, USA, Joined Mar 2000, 85

J. Mark Davis

Teacher, And Consultant
University of Ultrasonics, Birmingham, Alabama,
USA,
Joined Mar 2000
85
04:14 Feb-05-2000
Re: NDT of Polyurethane Foam
Dear Laurie,

I see you are at GM Delphi in Dayton. One of the NDT Process would be an automated ot semi-automated digital radiography system. I scanned some radiographs for a Tom Clark at Delphi last month. He can show you some of the digital images using our software. There in Dayton, you should contact Mr. Dennis Lee at US Inspection/Dayton X-ray. They will be able to help you out. (937) 228-9729.

You critical flaw size would not be a problem with digital radiuography. With the digitzed radiographs I can size flaws around 0.010 using geometric enlargment and using a calibrated RT ruler within the software.

Your parts would be put on a
tread mill and the parts would be moved through an X-ray system to greatly speed production. You could sample the parts or run them all.

Please email me if you have any other questions. The others who responded with Low freq. Ut and Thermograpgy are also very viable NDT methods.

As for cost I do not know.

Good Luck,

J. Mark Davis

: I work for Delphi Interior Systems near Dayton, Ohio. We make
: Instrument panels (dashboards) for automobiles using an injection
: molding process. This process involves injecting a polyurethane
: foam between layers of vinyl and a hard plastic shape retainer.
: When the parts are made, especially in the prototype stage, there
: are often voids in the foam that may not be detected by the eye
: or touch. I am looking for a way to detect the voids non-
: destrictively before shipping the parts to the customer. Ideally,
: I'd like to find a way to scan the parts and be able to create a
: mapping of where the voids occur, and how large they are.
: Typically, the voids that cause problems are anywhere from 7-10mm
: to a large hole that runs along the length of the part. Please
: let me know any ideas you may have, or if your company provides
: services and equipment to perform these tests.
: Thank you,
: Laurie Shopes
: Delphi Interior Systems




 
 Reply 
 
Malcolm woodhead
Malcolm woodhead
23:41 Jan-16-2020
Re: NDT of Polyurethane Foam
In Reply to Norm Woodward at 05:11 Feb-03-2000 .

I have a requirement to inspect a 8m x 2mx2m Polyurethane mould for voids prior to machining a surface and after machining. This must be a NDT process.

 
 Reply 
 
Johann Hinken
FI Test- und Messtechnik GmbH, Germany, Joined May 2014, 19

Johann Hinken

FI Test- und Messtechnik GmbH,
Germany,
Joined May 2014
19
09:51 Jan-20-2020
Re: NDT of Polyurethane Foam
In Reply to Malcolm woodhead at 23:41 Jan-16-2020 .

Hello, you should consider microwave testing. Please see for example
https://fitm.de/wp-content/uploads/2018/06/N38e_Microwave_Testing_An_Overview.pdf
If you have an initial interest in applying this method would like to give you more information.
Regards, Johann




 
 Reply 
 
Simon Amallraja
Consultant, Advanced NDT Methods
Anu Consultants, India, Joined Aug 2013, 40

Simon Amallraja

Consultant, Advanced NDT Methods
Anu Consultants,
India,
Joined Aug 2013
40
07:55 Feb-01-2020
Re: NDT of Polyurethane Foam
In Reply to Laurie Shopes at 05:30 Feb-01-2000 (Opening).

Hi,
Laser Shearography is ideally suited to this reqt. The defect sizes defined is achievable by this method. The 8 LD system can scan around 1800 mm x 1800 mm in single shot. You can fix the shear head in to any Robotic arm and the component can be tested - irrespective of shape and size.

if you are interested, email me and I will send more info on this applications.

 
 Reply 
 
Oleksandr Pogorielov
R & D,
sas BT2i , NDT Senior Advisor, Ukraine, Joined Dec 2010, 31

Oleksandr Pogorielov

R & D,
sas BT2i , NDT Senior Advisor,
Ukraine,
Joined Dec 2010
31
09:30 Feb-03-2020
Re: NDT of Polyurethane Foam
In Reply to Laurie Shopes at 05:30 Feb-01-2000 (Opening).

Try using the THz NDT method

For example - https://www.ndt.net/article/aero2010/papers/we4b3.pdf

 
 Reply 
 

Product Spotlight

Echomac® Small

Available with up to eight channels of electronics to detect and evaluate thickness, flaws and eccen
...
tricity, this UT tester is housed in a convenient, smaller cabinet. This instrument can be used in conjunction with bubbler or immersion tank systems, or with a test bench or in laboratory applications. The Echomac® Small is available in the FD4, FD6 or FD6A versions.
>

CIVA 2020 UT Module

CIVA NDE Simulation Software is the world leader of NDT Simulation. The UT simulation Module incl
...
udes: - "Beam computation": Beam propagation simulation - "Inspection Simulation": Beam interaction with flaws or specimens The user can simulate a whole inspection process (pulse echo, tandem or TOFD) with a wide range of probes (conventional, Phased- arrays or EMAT), components, and flaws.
>

Immersion systems

ScanMaster ultrasonic immersion systems are designed for high throughput, multi shift operation in a
...
n industrial or lab environment. These fully integrated systems provide various scanning configurations and incorporate conventional and phased arrays technologies to support diverse applications, such as inspection of disks, bars, shafts, billets and plates. All of ScanMaster immersion systems are built from high accuracy scanning frames allowing for scanning of complex parts and include a multi-channel ultrasonic instrument with exceptional performance. The systems are approved by all major manufacturers for C-scan inspection of jet engine forged discs. Together with a comprehensive set of software modules these flexible series of systems provide the customer with the best price performance solutions.
>

Magnetic X-Ray Pipeline Crawler

Zhong Yi brand pipeline crawler is magnetic/micro-video controlled crawler with DC X ray unit inst
...
alled for checking welding of pipeline. Move steadily inside the pipeline 6''-60''diameter with speed of up to 18m/min, Max. moving diatance 5 kilometers and provide the efficient inspection of the pipeline.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window