Dear Sirs

In our pipeline to the harbour, we have already done 100% visual inspection and manual UT. At the moment, to establish a true base line, we want to do a more reliable and conservative NDT testing.

Based on our pipeline description below we want to know, what are pipeline NDT inspection methods others than intrusive pig inspection to perform the job and how long it takes to accomplish such a work?

Our pipe way is composed by 14 straight lines 5,5Km length. In some points we have expansion loops with elbows. There are lines painted with an inorganic zinc primer plus an amine Epoxy 150u total thickness, other lines are painted with an alkyd red lead 80u. 36" and 30" lines are thermal insulated with rock wool and aluminium weatherproofing, the insulation has 50mm thickness, and these lines are steam heat traced. 10" Butane line is thermal insulated with 50mm of polyurethane. The lines have welded supports that are lying over concrete sleepers.

The forum answer will be appreciated.

Luis Marques.



 
 Reply 
 
John O'Brien
Consultant, -
Chevron ETC , USA, Joined Jan 2000, 283

John O'Brien

Consultant, -
Chevron ETC ,
USA,
Joined Jan 2000
283
01:44 Jan-20-2005
Re: pipeline NDT inspection methods others than intrusive pig inspection
A good approach may be to use Long Range Ultrasonics to screen substantial lengths of the pipeline. This would highlight areas requiring focussed NDE.

A broader approach maigh be a Risk Assessment comlemented by selected long range UT and then definitive inspection of identified fault areas.

Another alternative is EMAT screening of the pipe in those areas where the technique is suitable.

For more detail please feel free to contact me.


 
 Reply 
 
Vitali Grigil
Vitali Grigil
02:03 Jul-15-2008
Re: pipeline NDT inspection methods others than intrusive pig inspection
other alternatives could be magnetic methods and guided wave ultrasound.
Vitali Grigil

Transkor-USA, Inc.
Director

----------- Start Original Message -----------
: A good approach may be to use Long Range Ultrasonics to screen substantial lengths of the pipeline. This would highlight areas requiring focussed NDE.
: A broader approach maigh be a Risk Assessment comlemented by selected long range UT and then definitive inspection of identified fault areas.
: Another alternative is EMAT screening of the pipe in those areas where the technique is suitable.
: For more detail please feel free to contact me.
------------ End Original Message ------------




 
 Reply 
 
Vitali Grigil
Vitali Grigil
18:04 Mar-04-2010
Re: pipeline NDT inspection methods others than intrusive pig inspection
In Reply to Vitali Grigil at 02:03 Jul-15-2008 .

For more informationplease visit www.transkor-usa.com

 
 Reply 
 
Sang Kim
Consultant, NDT Trainer
Guided Wave Analysis LLC, USA, Joined Feb 2008, 44

Sang Kim

Consultant, NDT Trainer
Guided Wave Analysis LLC,
USA,
Joined Feb 2008
44
02:36 Mar-05-2010
Re: pipeline NDT inspection methods others than intrusive pig inspection
In Reply to Vitali Grigil at 18:04 Mar-04-2010 .

I also recommend to use long-range guided wave testing (GWT) for screening the pipeline. GWT is cost effective and can quickly screen long length of pipeline. If your pipeline includes geometric features such as pipe support, clamp, spacer, or wire tie, please use high-frequency guided wave that reduces the interaction of guided wave with attached geometric features. For learning more about this, please refer to this website ( http://www.gwanalysis.com/guided_wave_pipe_inspection.html ) or (http://www.ndt.net/forum/thread.php?admin=&forenID=1&msgID=32591&rootID=32547#32591).
If you know the resolution difference with 1 MHz, 2.25 MHz, 5 MHz, and 10 MHz transducers in UT inspection, you will realize that the high-frequency (frequency range between 100 kHz to 300 kHz) GWT is much better resolution in finding small defects than low-frequency (usually less than 50 kHz) GWT. High-frequency GWT has longer inspection range with high resolution than that of low-frequency GWT for a pipeline having many geometric features.

Sang Kim

 
 Reply 
 
mj
mj
09:06 Mar-05-2010
Re: pipeline NDT inspection methods others than intrusive pig inspection
In Reply to LUIS MARQUES at 00:59 Jan-20-2005 (Opening).

Dear Luis, as everybody said LRUT is the best method for this kind of pipeline, but you need to provide a good support with Manual UT, Pipeline with continues Welded support, Loops and Thick Coat Painting(External and Internal) not really good for LRUT, same like all other Inspections. 150 Micron thick external painting is ok. but most of the harbour line with high sludge/deposit inside will reduce your test range as well as quality of the inspection. Always reliable LRUT in this kind of piping inspection.

 
 Reply 
 
Florin Turcu
R & D
Dept. of Electrical Systems and Automation - University of Pisa, Italy, Joined Jul 2007, 9

Florin Turcu

R & D
Dept. of Electrical Systems and Automation - University of Pisa,
Italy,
Joined Jul 2007
9
10:56 Mar-09-2010
Re: pipeline NDT inspection methods others than intrusive pig inspection
In Reply to LUIS MARQUES at 00:59 Jan-20-2005 (Opening).

An idea would be to use Long Range Guided Waves for long term monitoring of your pipelines. Considering that you need anyway to remove the insulation in the locations where you'll install GW probes (over small areas though), it would be a good idea to install special probes that let you monitor that pipeline. This way, next time you won't have to remove insulation anymore, except for critical areas detected by GW monitoring.
Regards,
Florin Turcu, Pisa, Italy

 
 Reply 
 
Jesus Reynaldo
Bolivia, Joined Sep 2015, 1

Jesus Reynaldo

Bolivia,
Joined Sep 2015
1
14:13 Feb-15-2017
Re: pipeline NDT inspection methods others than intrusive pig inspection
In Reply to LUIS MARQUES at 00:59 Jan-20-2005 (Opening).

Dear Luis Markes,

Dis you made the test with MTM?, may you share your experience with us please.

 
 Reply 
 
Andreas Boenisch
Director,
Innospection Ltd., United Kingdom, Joined Aug 2011, 1

Andreas Boenisch

Director,
Innospection Ltd.,
United Kingdom,
Joined Aug 2011
1
11:27 Feb-20-2017
Re: pipeline NDT inspection methods others than intrusive pig inspection
In Reply to LUIS MARQUES at 00:59 Jan-20-2005 (Opening).

an alternative are the MEC (Magnetic Eddy Current) scanner systems (top side & subsea). a fast scanning with high resolution corrosion mapping externally and internally.
Typical speed 0.2m/sec., sensitive detecting small volumetric pitting and size it.
The scanners are used for coated subsea pipeline, riser, caisson and conductor inspection. Data prepared and direct transferred to an FFS system .

Let me know if interested in more information a.boenisch@innospection.com

 
 Reply 
 
Guennadi Krivoi
Guennadi Krivoi
08:58 Feb-21-2017
Re: pipeline NDT inspection methods others than intrusive pig inspection
In Reply to LUIS MARQUES at 00:59 Jan-20-2005 (Opening).

Another possible inspection technique which can be applied for ranges without aluminium weatherproofing is so-called AGIT (Above-Ground Inspection Technique) which can detect inner and outer metal loss faults. The inspection speed is about 1 m in 40 s, the pipeline range under test must be connected at the start and end positions to a special generator providing an AC test current into the pipeline. The inspection tool measures the outer AC magnetic field induced by the test current at different frequencies. The product transportation mode must not be stopped or even changed during the inspection.

For more details please feel free to contact me under the address: krivoi@empit.com

 
 Reply 
 

Product Spotlight

Research Center IDEKO develops an ultrasonic train wheel inspection system for CAF

The Basque Research centre IK4-IDEKO has developed a state-of-the-art ultrasonic inspection system f
...
or the train wheel. This system secures a sound condition of train wheels and is thus a significant contribution to rail transport safety. The device was delivered to CAF recently and its use allows the manufacturer to become an approved supplier of rolling stock in Italy, as it meets the demanding homologation standards of this country. \\\\r\\\\n
>

Extended Range Variable Wall® Piping Calibration Blocks for Longseam Inspection

This set of two blocks has been specially designed for situations where ultrasonic examination tak
...
es place circumferentially or “around the curve” for applications such as inspection of longseam welds in piping and vessels. Jointly designed by PH Tool and Holloway NDT, the blocks feature side-drilled hole reflectors positioned within novel compound-curves, each with multiple thickness steps. The unique design results in a light and compact form factor, with the largest block weighing just over 15 lbs and spanning just 16 ¾”. Coverage is provided for nominal pipe sizes from 6” to 10” in the small block and 12” to a whopping 56” in the large block. The compound OD curves and multiple wall thicknesses actually exceed ASME requirements, providing exceptional signal response and measurement accuracy. Properly managing beam divergence off the ID and stabilizing beam skew due to probe rocking is essential to maintaining a consistent calibration when inspecting lengthwise on curved surfaces.
>

GUL Subsea Solutions - Screeening & Monitoring

To inspect new and existing subsea lines, you need proven technology and experience. GUL offers it's
...
technology to solve this challenge: GUL Subsea and gMAT Transducer Rings.
>

IRIS 9000Plus - Introducing the next generation of heat exchanger inspection.

Representing the seventh generation of the IRIS system, the IRIS 9000 Plus has nearly 200 years of c
...
ombined field inspection experience incorporated in its design. This experience combined with a strong commitment to quality and a history of innovation has made Iris Inspection Services® the undisputed leader in IRIS technology.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window