Seamless pipe test.

Hi, Friendes

I want to test the seamless pipe by ultrasonic contact type method.

To cover the maximum area

# I am using the angle probe 45 degree and 4 MHz and crystal size is 8x 9 mm and the beam spread is approx. 5 degree. As per my knoledge the effective beam width of this probe is Less Is it right ?

# Can i use the 10 mm dia lonitudinal beam probe with the angulated wadge ( angle is 45 degree ) ? In this case can i get the more effective beam width ?

Please Help to sort out my purpose. Thanking you.

S.G.




 
 Reply 
 
Ed T.
Ed T.
03:07 Sep-29-2004
Re: Seamless pipe test.
----------- Start Original Message -----------
: Hi, Friendes
: I want to test the seamless pipe by ultrasonic contact type method.
: To cover the maximum area
: # I am using the angle probe 45 degree and 4 MHz and crystal size is 8x 9 mm and the beam spread is approx. 5 degree. As per my knoledge the effective beam width of this probe is Less Is it right ?
: # Can i use the 10 mm dia lonitudinal beam probe with the angulated wadge ( angle is 45 degree ) ? In this case can i get the more effective beam width ?
: Please Help to sort out my purpose. Thanking you.
: S.G.
------------ End Original Message ------------

Can you be more specific? What exactly are you testing the seamless pipe for? Is there a girth weld involved?
What exactly are you trying to detect?



 
 Reply 
 
S.G.
Consultant
Enrico Enterprises, India, Joined Jul 2004, 20

S.G.

Consultant
Enrico Enterprises,
India,
Joined Jul 2004
20
05:46 Sep-30-2004
Re: Seamless pipe test.
----------- Start Original Message -----------
: : Hi, Friendes
: : I want to test the seamless pipe by ultrasonic contact type method.
: : To cover the maximum area
: : # I am using the angle probe 45 degree and 4 MHz and crystal size is 8x 9 mm and the beam spread is approx. 5 degree. As per my knoledge the effective beam width of this probe is Less Is it right ?
: : # Can i use the 10 mm dia lonitudinal beam probe with the angulated wadge ( angle is 45 degree ) ? In this case can i get the more effective beam width ?
: : Please Help to sort out my purpose. Thanking you.
: : S.G.
: Can you be more specific? What exactly are you testing the seamless pipe for? Is there a girth weld involved?
: What exactly are you trying to detect?
------------ End Original Message ------------

The defect is N5 notch and wall thickness is 5 mm to 15 mm. There is no weld nothing.




 
 Reply 
 
Neil Burleigh
Sales
Krautkramer Australia Pty Ltd, Australia, Joined Dec 2002, 158

Neil Burleigh

Sales
Krautkramer Australia Pty Ltd,
Australia,
Joined Dec 2002
158
07:16 Oct-05-2004
Re: Seamless pipe test.
Hello Shashu,
The formula for the determination of beam width Y = arc sin1.22(wavelength/diameter)
Which means that as the diameter of the crystal increases the beam width at a certain beam path length will decrease.
Are you trying to detect the N5 notch radially as well as longitudinally?
The diameter of the pipe will affect the beam spread and beam angle when testing longitudinally.
Will you be shaping the probe shoe to the contour of the pipe?

Regards

Neil Burleigh


----------- Start Original Message -----------
: : : Hi, Friendes
: : : I want to test the seamless pipe by ultrasonic contact type method.
: : : To cover the maximum area
: : : # I am using the angle probe 45 degree and 4 MHz and crystal size is 8x 9 mm and the beam spread is approx. 5 degree. As per my knoledge the effective beam width of this probe is Less Is it right ?
: : : # Can i use the 10 mm dia lonitudinal beam probe with the angulated wadge ( angle is 45 degree ) ? In this case can i get themore effective beam width ?
: : : Please Help to sort out my purpose. Thanking you.
: : : S.G.
: : Can you be more specific? What exactly are you testing the seamless pipe for? Is there a girth weld involved?
: : What exactly are you trying to detect?
: The defect is N5 notch and wall thickness is 5 mm to 15 mm. There is no weld nothing.
------------ End Original Message ------------




 
 Reply 
 
akin nowahalla
akin nowahalla
08:25 May-19-2005
Re: use of Seamless pipe
please possible to tell me what is used to produce seamless pipe/steel and what do we use this pipes/steels for.

thanks/me.


 
 Reply 
 

Product Spotlight

NDT Master Lecturer

In the program both university professors and practitioners will give lectures, which guarantees the
...
oretical depth and practical inside. Academic Director: Prof. Dr. Christian Boller
The following lecturers are not complete: Prof. Tadeusz Stepinski, Prof. Wieslaw Staszewski, Prof. Frank Walther, Prof. Giovanni Bruno, Prof. Gerd Dobmann, Prof. Philippe Guy
>

YXLON Cougar EVO

Scalable small footprint X-ray inspection systems for assembly and laboratory applications. The
...
YXLON Cougar EVO series was designed to provide the "best-in- class" inspection solutions for SMT, semiconductor, and laboratory assembly applications, while maintaining a small system footprint for maximum convenience. With optimized software and hardware, these systems produce higher quality and more consistent results than other electronics inspection systems currently on the market.
>

IntraPhase Athena Phased Array System

The Athena Phased Array system, manufactured by WesDyne NDE Products & Technology, consists of a pha
...
sed array acquisition system and PC running IntraSpect software. A PC is used to perform acquisition, analysis and storage of the data. System hardware is capable of operating up to four data sets with any combination of phased array or conventional UT probes. NOW AVAILABLE IN 64-64 CONFIGURATION.
>

FAAST-PA! OEM Patented phased Array for high speed UT inspection

Multiangle, Multifocus, Multifrequency, Multibeam. Instead of stacking UT electronics and having m
...
any PA probes, FAAST-PA is able to transmit all delay laws within ONE single shot in Real time.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window