25 kV overhead hard drawn Copper Contact wire

We are facing the problem of unexplained breakage of contact wire
of 107 square millimeter ( one fourth of a square inch ) which is kept
under 1000 Kg ( 2240 pounds ) tension.
It carries current to electric locomotives through a Pantograph
which maintains 7 Kg pressure.
Any suggestions for preventive diagonostics and testing of contact
wire before stringing ?
Dinesh Bansal, Chennai ( Madras ) , India



 
 Reply 
 
Godfrey Hands
Consultant,
PRI Nadcap, United Kingdom, Joined Nov 1998, 307

Godfrey Hands

Consultant,
PRI Nadcap,
United Kingdom,
Joined Nov 1998
307
08:17 Jun-14-1999
Re: 25 kV overhead hard drawn Copper Contact wire
: We are facing the problem of unexplained breakage of contact wire
: of 107 square millimeter ( one fourth of a square inch ) which is kept
: under 1000 Kg ( 2240 pounds ) tension.
: It carries current to electric locomotives through a Pantograph
: which maintains 7 Kg pressure.
: Any suggestions for preventive diagonostics and testing of contact
: wire before stringing ?
: Dinesh Bansal, Chennai ( Madras ) , India
:

Hallo Mr. Bansal.
I suggest that the copper wire is eddy current tested before installing. Use this to detect cracks and splits in the wire, and also to detect local inhomogenieties in the wire.
Is the supplier in India or elsewhere in the world. You may be able to specify tested wire in yiour purchase.
The problem may also be caused by local arc burning of the wire from disconnections and recommections of the locomotives whilst in service.

Regards
Godfrey Hands



 
 Reply 
 
Siamak Shokri (Msc in metallurgical Engineering)
Siamak Shokri (Msc in metallurgical Engineering)
04:07 Aug-14-2000
Re: 25 kV overhead hard drawn Copper Contact wire
We are looking for production of grooved contact wire in Railways research center of Iran.We need some information about production of it.we will be glad if you send us this information or introduce us to suppliers of this type of wires.
our address is:
Iran Railways research center,production group
no.201 Italia crossing,Vessal avenue
Tehran,Iran
Fax no. 009821-651462
Yours Faithful



 
 Reply 
 

Product Spotlight

ISAFE3 Intrinsically Safe Sensor System

ISAFE3 intrinsically safe sensor system of Vallen Systeme is especially targeted at the petrochemica
...
l - as well as oil and gas transportation industry. The sensor system is designed for permanent monitoring or periodic inspection tasks. Sensors are available for different AE-frequency ranges optimized for corrosion and fatigue crack detection and other applications. The ISAFE 3 sensor system consists of an AE-sensor (model ISAS3) certified according to ATEX/IEC for installation in zone 0, gas group IIC, IP68, 20 to +60 °C, and a signal isolator (model SISO3) certified for installation in zone 2. An ISAS3 sensor can be mounted in atmosphere or submerged, e.g. in water or crude oil. It is supported by mounting tools for temporary (magnets) or permanent (welded) installation. ISAFE3 supports automatic sensor coupling test and can be used with any AE signal processor supporting 28V supply at 90 mA peak, e.g. Vallen Systeme ASIP-2/A.
>

ISONIC 3510

Very Powerful Superior Performance Extremely Portable Smart Phased Array Ultrasonic Flaw Detector an
...
d Recorder with 2 Conventional UT and TOFD Channels uniquely combines PA, single- and multi-channel conventional UT, and TOFD modalities providing 100% raw data recording and imaging. Suitable for all kinds of every-day ultrasonic inspections
>

NOVO Armor 15 & NOVO Armor 22

The Armor Kit Contains the NOVO Armor, which provides additional mechanical protection to the NOVO 1
...
5WN & NOVO 22WN Detectors, the Armor Stand and a traveling soft cover. - Newest shock absorbent technology case - Water resistant design - Supports wired & wireless communication - Multiple positioning options - Tripod connection using the Built-in 1/4” threads - Simple Detector battery replacement
>

Customized Probes and Transducers

With a strong development department and our own piezocomposite production, we accompany you from th
...
e first product idea to serial production. Our scientists are continuously researching new methods in the field of ultrasonic measurement technology. The progress achieved enables us to offer you optimal solutions.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window