Charlie Jackson
Charlie Jackson
02:09 Mar-20-2006
UT Flaw detection in Monel and Hastelloy weldments

Interested to know of any UT Techniques for Monel or Hastelloy weldments which would give a reasonable POD for preferential ID corrosion loss to Weld or HAZ in piping.

Kind Regards Charlie


 
 Reply 
 
Frank
Frank
05:35 Mar-25-2006
Re: UT Flaw detection in Monel and Hastelloy weldments
----------- Start Original Message -----------
: Interested to know of any UT Techniques for Monel or Hastelloy weldments which would give a reasonable POD for preferential ID corrosion loss to Weld or HAZ in piping.
: Kind Regards Charlie
------------ End Original Message ------------

Try using Refracted Longitudinal search units.


 
 Reply 
 
Jim Knowles
Jim Knowles
00:12 Mar-28-2006
Re: UT Flaw detection in Monel and Hastelloy weldments
----------- Start Original Message -----------
: : Interested to know of any UT Techniques for Monel or Hastelloy weldments which would give a reasonable POD for preferential ID corrosion loss to Weld or HAZ in piping.
: : Kind Regards Charlie
: Try using Refracted Longitudinal search units.
------------ End Original Message ------------


The corrosion of this type can be put into three categories,notch, U type or escarpment, two can be detected relatively easily by a 45 degree shear either 0.5 skip or multiple skip paying attention to the particular area of impingement or beam path length. The escarpment type of geometry is more difficult as it is shallow from the pipe side gradually getting deeper nearer the weld or HAZ. Try using 4.0 MHz shear or if the material is partcularly noisy angled compression as Charlie recommends.



 
 Reply 
 
J. Mark Davis
Teacher, And Consultant
University of Ultrasonics, Birmingham, Alabama, USA, Joined Mar 2000, 85

J. Mark Davis

Teacher, And Consultant
University of Ultrasonics, Birmingham, Alabama,
USA,
Joined Mar 2000
85
04:21 Mar-28-2006
Re: UT Flaw detection in Monel and Hastelloy weldments
IS this just corrosion or is ID cracking a concern.

Refracted Longitudinal Waves may work and even ID Creeping Waves.

Phased Array UT is another consideration. Either a E Scan or a S-Scan could image the sorroded area.

Is there any weld crown restriction?

How thick is the Hastelloy and Monel material?

J. Mark Davis

----------- Start Original Message -----------
: : Interested to know of any UT Techniques for Monel or Hastelloy weldments which would give a reasonable POD for preferential ID corrosion loss to Weld or HAZ in piping.
: : Kind Regards Charlie
: Try using Refracted Longitudinal search units.
------------ End Original Message ------------




 
 Reply 
 

Product Spotlight

NEW Wheel Type Phased Array Probe

DOPPLER NEW Wheel Type Phased Array Probe, more stable, new tyre makes lesser acoustic attenuation
...
, much lighter makes easier to handle, more slim size, magnetic and mechanical encoder optional etc...more
>

MUSE Mobile Ultrasonic Equipment

The MUSE, a portable ultrasonic imaging system, was developed for in-field inspections of light-weig
...
ht structures. The MUSE consists of a motor-driven manipulator, a water circulation system for the acoustic coupling and a portable ultrasonic flaw detector (USPC 3010). The MUSE provides images of internal defects (A-, B-,C- and D-scan).
>

PAUT Probes

Typical Phased Array probes have frequencies between 1MHz and 20MHz and the number of wafers is 10
...
to 128. M2 Electronics offers customers conventionally ultrasound probes and the ability to provide high-precision Phased Array Ultrasound Probes of up to 256 wafers. We can also customize the probe for our customers to meet the specific application requirements of the user.
>

Conformable wedge transducer

The conformability is obtained with a flexible membrane filled with water between the transducer and
...
the inspected component. The coupling between the membrane and the component requires a small quantity of water or couplant. The conformable wedge combines the acoustic performance of immersion technique with good coupling and low attenuation.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window