UT Longitudional Wave Velocity Tables

To all:

Does anyone know of a web-site or source where I can obtain Ultrasonic Longitudional Wave Velocities for the following materials?

1) Carbon Steel(B)
2) Cr - 1/2 Mo Steel (T1 or P1)
3) 1-1/4 Cr - 1/2 Mo Steel (T11 or P11)
4) 2-1/4 Cr - 1 Mo Steel (T22 or P22)
5) 3 Cr - 1 Mo Steel (T21 or P21)
6) 5 Cr - 1/2 Mo Steel (T5 or P5)
7) 5 Cr - 1/2 Mo-Si Steel (T5b or P5b)
8) 7 Cr - 1/2 Mo Steel (T7 or P7)
9) 9 Cr - 1 Mo Steel (T9 or P9)
10) 9 Cr - 1 Mo-Va Steel (T91 or P91)
11) 18 Cr - 8 Ni Steel (304 or 304H)
12) 16 Cr - 12 Ni - 2 Mo Steel (316 or 316H)
13) 16 Cr - 12 Ni - 2 Mo Steel (316L)
14) 18 Cr - 10 Ni - Ti Steel (321 or 321H)
15) 18 Cr - 10 NiCb Steel (347 or 347H)
16) Ni-Fe-Cr (Alloy 800H)
17) 25 Cr - 20 Ni (HK-40)

All assistance is greatly appreciated.
Regards, Rich



 
 Reply 
 
Don
Don
00:56 Aug-11-2004
Re: UT Longitudional Wave Velocity Tables
You can calculate the Longitudinal (compression) wave velocity is you know values for the Modulus of elasticity (E), Density(p) and Poisson's ratio(u) of the material.
It is given by the equation:-

VLong=SQRT( E(1-u) / p(1+u)(1-2u) )

If these are not known, a good source of info if the CNDE site at IOWA university

Don


----------- Start Original Message -----------
: To all:
: Does anyone know of a web-site or source where I can obtain Ultrasonic Longitudional Wave Velocities for the following materials?
: 1) Carbon Steel(B)
: 2) Cr - 1/2 Mo Steel (T1 or P1)
: 3) 1-1/4 Cr - 1/2 Mo Steel (T11 or P11)
: 4) 2-1/4 Cr - 1 Mo Steel (T22 or P22)
: 5) 3 Cr - 1 Mo Steel (T21 or P21)
: 6) 5 Cr - 1/2 Mo Steel (T5 or P5)
: 7) 5 Cr - 1/2 Mo-Si Steel (T5b or P5b)
: 8) 7 Cr - 1/2 Mo Steel (T7 or P7)
: 9) 9 Cr - 1 Mo Steel (T9 or P9)
: 10) 9 Cr - 1 Mo-Va Steel (T91 or P91)
: 11) 18 Cr - 8 Ni Steel (304 or 304H)
: 12) 16 Cr - 12 Ni - 2 Mo Steel (316 or 316H)
: 13) 16 Cr - 12 Ni - 2 Mo Steel (316L)
: 14) 18 Cr - 10 Ni - Ti Steel (321 or 321H)
: 15) 18 Cr - 10 NiCb Steel (347 or 347H)
: 16) Ni-Fe-Cr (Alloy 800H)
: 17) 25 Cr - 20 Ni (HK-40)
: All assistance is greatly appreciated.
: Regards, Rich
------------ End Original Message ------------





 
 Reply 
 
m.prabhakaran
m.prabhakaran
01:11 Oct-07-2004
Re: UT Longitudional Wave Velocity Tables
respected sir
i am in need of 9 Cr - 1 Mo Steel (T9 or P9) composition and basic behind that,pls send me to my email id



 
 Reply 
 

Product Spotlight

ISAFE3 Intrinsically Safe Sensor System

ISAFE3 intrinsically safe sensor system of Vallen Systeme is especially targeted at the petrochemica
...
l - as well as oil and gas transportation industry. The sensor system is designed for permanent monitoring or periodic inspection tasks. Sensors are available for different AE-frequency ranges optimized for corrosion and fatigue crack detection and other applications. The ISAFE 3 sensor system consists of an AE-sensor (model ISAS3) certified according to ATEX/IEC for installation in zone 0, gas group IIC, IP68, 20 to +60 °C, and a signal isolator (model SISO3) certified for installation in zone 2. An ISAS3 sensor can be mounted in atmosphere or submerged, e.g. in water or crude oil. It is supported by mounting tools for temporary (magnets) or permanent (welded) installation. ISAFE3 supports automatic sensor coupling test and can be used with any AE signal processor supporting 28V supply at 90 mA peak, e.g. Vallen Systeme ASIP-2/A.
>

OPBOX with standard software is able to do all types of inspections and measurements: flaw detection in welds and materials, scanning of objects, testing composite materials, forged and moulded pieces, many UT inspections, measurements of properties of ma

Typical applications: UT measurements with pulse technique, Measurement of thicknesses also at hig
...
h temperatures, Measurements of properties of materials, including fluids and gases We are delivering a standard version of the software (for any Microsoft Windows up to 10 x64 with Microsoft Hardware certification report Approved) and for special needs: SDK with ready to use examples for LabView, MATLAB x64, C++ wrapper for dll, Python and Linux., and also low-level description of how to control our devices directly from any USB tools
>

Varex Imaging Large Field of View (FOV) Digital Detector Arrays (DDAs)

A larger FOV DDA can reduce the space and volume of the X-ray inspection system on the factory floor
...
, enable faster scanning times, better throughput and better resolution images at a lower dose. Customers can also save time and money. With these benefits in mind, Varex Imaging has designed a family of large FOV detectors (4343HE, XRD 1611, 4343DX-I, 4343CT) for our industrial imaging customers.
>

NDTkit RT

NDTkit RT, TESTIA's Digital Radiography software The NDTkit product line software for X-ray analysi
...
s. NDTkit RT is a software benefiting from the Ultis kernel which is dedicated to radiographic image analysis. It offers a set of tools and filtering processes to assist RT operators in finding relevant flaws.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window